A bolting specification tells you more than how strong a stud is. It sets the chemistry, the heat treatment, the testing, the marking and the service the bolting is meant for. This guide explains how ASTM, SAE and metric (ISO) bolting specifications are organized, what the grade and class numbers mean, how to read the markings, and how the common grades compare.
- Reading a callout
- Who writes the specs
- ASTM A193 and A320
- A194 nuts
- ASTM general and structural
- SAE J429
- Metric classes
- Stainless and nickel
- Comparing grades
- Markings
- Ordering checklist
How to read a bolting callout
A complete bolting description has several parts, and each one matters. The specification names the document that sets the requirements. The grade sets the chemistry and heat treatment. For some materials, such as strain-hardened stainless, a class sets the strength level. Size, thread and length come from separate dimensional standards, and the nut is a separate specification with its own grade.
Figure 1
Anatomy of a bolting order line
Material specifications are separate from dimensional standards. ASTM A193 says what a B7 stud is made of and how it is tested. ASME B1.1 sets the thread, ASME B18.2.1 and B18.2.2 set bolt head and nut dimensions, and ASME B16.5 sets which stud size and length a flange needs. Use our stud bolt length calculator for the last one.
Who writes bolting specifications
Some ASTM specifications cover inch and metric sizes in one document, such as F3125, which has Grades A325 (120 ksi) and A325M (830 MPa). Others come as pairs, such as A193 and A193M. The M version uses the same grade names with SI units and metric threads, so an A193M B7 stud is still a B7 stud.
ASTM pressure and temperature bolting
These are the specifications called out by piping and pressure vessel codes for flanged joints in refineries, chemical plants and power plants. Strength minimums for quenched and tempered grades fall with diameter because large bars cannot be hardened as deeply. Markings for the most common grades are on our Bolting Grades and Markings sheet.
ASTM A193 ferritic (alloy and martensitic) grades
| Grade | Material | Size, in. | Tensile / yield, min (ksi) | Hardness, max | Typical A194 nut |
|---|---|---|---|---|---|
| B5 | 5% chromium steel (4 to 6% Cr, 501 type), Q&T | To 4 | 100 / 80 | – | 3 |
| B6 | 12% chromium stainless (410, S41000), Q&T | To 4 | 110 / 85 | – | 6 or 6F |
| B6X | 410 stainless, lower strength, hardness limited | To 4 | 90 / 70 | 26 HRC | 6 or 6F |
| B7 | Cr-Mo alloy steel (4140 / 4142 / 4145), Q&T | To 2-1/2 Over 2-1/2 to 4 Over 4 to 7 | 125 / 105 115 / 95 100 / 75 | 321 HBW or 35 HRC | 2H or 7 |
| B7M | B7 chemistry, tempered at 1,150 °F min, 100% hardness tested | To 4 Over 4 to 7 | 100 / 80 100 / 75 | 235 HBW or 99 HRB | 2HM or 7M |
| B16 | Cr-Mo-V alloy steel, Q&T at 1,200 °F min | To 2-1/2 Over 2-1/2 to 4 Over 4 to 8 | 125 / 105 110 / 95 100 / 85 | 321 HBW or 35 HRC | 7 or 16 |
ASTM A193 austenitic (stainless) grades
A193 lists fourteen austenitic grade families. The letters after B8 identify the alloy: C for 347, T for 321, M for 316, P for 305, N for nitrogen-strengthened, L for low carbon, and a trailing A for material solution treated after machining. Every stainless grade must be ordered with a class.
| Grade | Type | UNS | Classes available | Matching A194 nut |
|---|---|---|---|---|
| B8, B8A | 304 | S30400 | 1, 1A, 1D, 2, 2B | 8, 8A |
| B8C, B8CA | 347 (niobium stabilized) | S34700 | 1, 1A, 1D, 2 | 8C, 8CA |
| B8M, B8MA, B8M2, B8M3 | 316 | S31600 | 1, 1A, 1D, 2 (B8M2: 2B; B8M3: 2C) | 8M, 8MA |
| B8P, B8PA | 305 | S30500 | 1, 1A, 1D, 2 | 8P, 8PA |
| B8T, B8TA | 321 (titanium stabilized) | S32100 | 1, 1A, 2 | 8T, 8TA |
| B8N, B8NA | 304N | S30451 | 1A, 1B, 1D, 2 | 8N, 8NA |
| B8MN, B8MNA | 316N | S31651 | 1A, 1B, 1D, 2 | 8MN, 8MNA |
| B8LN, B8LNA | 304LN | S30453 | 1, 1A, 1D | 8LN, 8LNA |
| B8MLN, B8MLNA | 316LN | S31653 | 1, 1A, 1D | 8MLN, 8MLNA |
| B8CLN, B8CLNA | 347LN | S34751 | 1, 1A, 1D | 8CLN, 8CLNA |
| B8MLCuN, B8MLCuNA | 6% Mo super austenitic | S31254 | 1A, 1B, 1D, 2 | 8MLCuN, 8MLCuNA |
| B8ML4CuN, B8ML4CuNA | 317-type, high Mo | S31730 | 1, 1A, 1D | 8ML4CuN, 8ML4CuNA |
| B8R, B8RA | XM-19, high nitrogen | S20910 | 1C, 1D | 8R, 8RA |
| B8S, B8SA | High-silicon, galling resistant | S21800 | 1C, 1D | 8S, 8SA |
What the stainless classes mean
| Class | Condition | Grades | Tensile / yield, min (ksi) |
|---|---|---|---|
| 1 | Carbide solution treated | B8, B8M, B8P, B8C, B8T, B8LN, B8MLN, B8CLN B8ML4CuN | 75 / 30, all sizes (223 HBW max) 70 / 25 |
| 1A | Solution treated in the finished condition (after machining and threading) for best corrosion resistance | All “A” grades, such as B8A, B8MA, B8CA, B8TA | 75 / 30, all sizes (192 HBW max); B8ML4CuNA 70 / 25 |
| 1B | Carbide solution treated, nitrogen-bearing grades | B8N, B8MN, B8MLCuN | 80 / 35, all sizes |
| 1C | Carbide solution treated, high-strength nitrogen grades | B8R, B8RA B8S, B8SA | 100 / 55 95 / 50 (271 HBW max) |
| 1D | Solution treated by rapid cooling from the hot-rolling temperature; limited to service below 850 °F | B8, B8M, B8P, B8LN, B8MLN, B8CLN, B8N, B8MN, B8MLCuN, B8R, B8S | Same as the matching Class 1, 1B or 1C grade |
| 2 | Solution treated and strain hardened | B8, B8C, B8P, B8T, B8N B8M, B8MN, B8MLCuN | 125 / 100 to 3/4 in., falling to 100 / 50 at 1-1/2 in. 110 / 95 to 3/4 in., falling to 90 / 50 at 1-1/2 in. |
| 2B | Solution treated and strain hardened, larger sizes | B8, B8M2 | 95 / 75 to 2 in.; 90 / 65 to 2-1/2 in.; 80 / 55 to 3 in. |
| 2C | Solution treated and lightly strain hardened | B8M3 | 85 / 65 to 2 in.; 85 / 60 over 2 in. |
Strain-hardened Class 2, 2B and 2C stainless may not have uniform properties through the section, especially over 3/4 in. diameter. At 1-1/2 in. and larger, core properties may be lower than test results taken at half radius.
ASTM A320 and other pressure bolting
| Spec and grade | Material | Tensile / yield, min (ksi) | Typical A194 nut | Typical use |
|---|---|---|---|---|
| ASTM A320: low-temperature service (impact tested) | ||||
| L7 | Cr-Mo alloy steel, Q&T | 125 / 105 to 2-1/2 in. | 7 (7L when impact tested) | Impact tested at −150 °F |
| L7M | Cr-Mo alloy steel, hardness limited | 100 / 80 to 2-1/2 in. | 7M (7ML when impact tested) | Low temperature and sour service |
| L43 | Ni-Cr-Mo alloy steel (4340), Q&T | 125 / 105 to 4 in. | 7 or 43 | Heavy sections at low temperature |
| Other pressure and special bolting | ||||
| A453 Gr 660 | A-286 iron-base superalloy, precipitation hardened | 130 / 85 (Classes A, B) | A453 660 nuts | High temperature and high strength |
| A540 | Special alloy steel, Grades B21 to B24 | Set by class | A540 nuts | Critical service such as turbines and nuclear components |
ASTM A194 nut grades
ASTM A194 covers the heavy hex nuts used with A193, A320 and A453 bolting. The nut grade number usually mirrors the stud grade: 2H or 7 for B7, 2HM or 7M for B7M, 8M for B8M. Proof stress is the load the nut must carry without stripping or permanent set, divided by the stress area of the mating bolt.
| A194 grade | Material | Condition | Proof stress, heavy hex (ksi) | Pairs with |
|---|---|---|---|---|
| Carbon and alloy steel (ferritic) | ||||
| 1 | Carbon steel | As forged or machined | 130 | Low-strength general bolting |
| 2 | Medium carbon steel | Not quenched and tempered | 150 | Older carbon steel bolting |
| 2H | Medium carbon steel | Quenched and tempered (248 to 327 HBW to 1-1/2 in.) | 175 | A193 B7, B16; A320 L7 |
| 2HM | Medium carbon steel | Q&T, hardness limited to 159 to 235 HBW, 100% tested | 150 | A193 B7M; A320 L7M (sour service) |
| 3 | Type 501 (5% Cr) steel | Quenched and tempered | 175 | A193 B5 |
| 6, 6F | 410 stainless (6F: 416 free machining) | Q&T, 228 to 271 HBW | 150 | A193 B6, B6X |
| 7 | Cr-Mo alloy steel (4140 family) | Quenched and tempered | 175 | A193 B7, B16; A320 L7, L43 |
| 7M | Cr-Mo alloy steel | Q&T, hardness limited to 159 to 235 HBW, 100% tested | 150 | A193 B7M; A320 L7M |
| 16 | Cr-Mo-V alloy steel | Quenched and tempered | 175 | A193 B16 |
| 43 | Ni-Cr-Mo alloy steel (4340) | Quenched and tempered (recent editions) | 175 | A320 L43 |
| 4 | Carbon-molybdenum steel | Withdrawn in 2017; still seen on older drawings | 175 | Replace with Grade 7 when allowed |
| Stainless and super austenitic (all 80 ksi proof) | ||||
| 8, 8A | 304 (S30400) | 8: solution treated, 126 to 300 HBW 8A: solution treated after finishing, 126 to 192 HBW | 80 | A193 B8, B8A |
| 8M, 8MA | 316 (S31600) | Same as 8 / 8A | 80 | A193 B8M, B8MA |
| 8C, 8CA | 347 (S34700) | Same as 8 / 8A | 80 | A193 B8C, B8CA |
| 8T, 8TA | 321 (S32100) | Same as 8 / 8A | 80 | A193 B8T, B8TA |
| 8F, 8FA | 303 free machining (S30300) | Same as 8 / 8A | 80 | General stainless bolting |
| 8P, 8PA | 305 (S30500) | Same as 8 / 8A | 80 | A193 B8P, B8PA |
| 8N, 8NA / 8MN, 8MNA | 304N (S30451) / 316N (S31651) | Same as 8 / 8A | 80 | A193 B8N, B8MN |
| 8LN, 8LNA / 8MLN, 8MLNA | 304LN (S30453) / 316LN (S31653) | Same as 8 / 8A | 80 | A193 B8LN, B8MLN |
| 8CLN, 8CLNA | 347LN (S34751) | Same as 8 / 8A | 80 | A193 B8CLN |
| 8MLCuN, 8MLCuNA | 6% Mo super austenitic (S31254) | Same as 8 / 8A | 80 | A193 B8MLCuN |
| 8ML4CuN, 8ML4CuNA | 317-type (S31730) | Same as 8 / 8A | 80 | A193 B8ML4CuN |
| 8R, 8RA | XM-19 (S20910) | 183 to 271 HBW | 80 | A193 B8R, B8RA |
| 8S, 8SA | High-silicon austenitic (S21800) | 183 to 271 HBW | 80 | A193 B8S, B8SA |
| 9C, 9CA | 6% Mo super austenitic (N08367) | Same as 8 / 8A | 80 | Super austenitic stud bolting |
Every A194 nut carries the grade and the manufacturer’s mark on one face. A “B” is added when the nut is machined from bar, an “A” marks stainless nuts solution treated after finishing, and an “L” suffix (such as 7L) marks nuts that are impact tested for low-temperature service. For sour service, the 2HM and 7M hardness limits apply. See the Sour Service Bolting Quick Reference. Pairings shown are common practice; the governing code and the purchaser’s specification decide the required nut grade.
ASTM general, structural and anchor bolting
These specifications cover machinery, structural steel and foundation bolting. They are paired with ASTM A563 nuts and, for structural work, ASTM F436 hardened washers.
| Spec and grade | Material | Tensile / yield, min (ksi) | Typical nut | Typical use |
|---|---|---|---|---|
| A307 Gr A / B | Low-carbon steel | 60 tensile (Gr B 60 to 100) | A563 A | General bolting; Gr B for cast-iron flanges |
| A449 | Medium-carbon or alloy steel, Q&T | 120 / 92 to 1 in.; 105 / 81 to 1-1/2 in.; 90 / 58 to 3 in. | A563 DH (galvanized) | Grade 5 strength in sizes to 3 in. |
| A354 BC | Alloy steel, Q&T | 125 / 109 to 2-1/2 in.; 115 / 99 to 4 in. | A563 C | Medium-high strength studs and rods |
| A354 BD | Alloy steel, Q&T | 150 / 130 to 2-1/2 in.; 140 / 115 to 4 in. | A563 DH | Grade 8 strength in sizes to 4 in. |
| F3125 A325 | Carbon or alloy steel, Q&T (Type 1 or 3) | 120 / 92 | A563 DH or A194 2H | Structural steel connections, 1/2 to 1-1/2 in. |
| F3125 A490 | Alloy steel, Q&T (Type 1 or 3) | 150 to 173 / 130 | A563 DH or A194 2H | High-strength structural connections |
| F1554 Gr 36 / 55 / 105 | Carbon or alloy steel anchor rods | Yield 36, 55 or 105 (the grade number) | A563 A or DH | Anchor rods cast into concrete |
F3125 replaced six older specifications in 2015, including A325 and A490, which are now grades within it. A325 is 120 ksi for all diameters to 1-1/2 in. The current edition also adds a 144 ksi class.
SAE J429 inch grades
SAE J429 is the familiar Grade 2, 5 and 8 system for inch hex cap screws and bolts in machinery and equipment. It stops at 1-1/2 in. Above that size, ASTM A449 is the usual Grade 5 equivalent and A354 BD the usual Grade 8 equivalent. Matching nuts are SAE J995 of the same grade.
| Grade | Size, in. | Proof (ksi) | Yield, min (ksi) | Tensile, min (ksi) | Head marking | Material |
|---|---|---|---|---|---|---|
| 1 | 1/4 to 1-1/2 | 33 | 36 | 60 | None | Low or medium carbon steel |
| 2 | 1/4 to 3/4 | 55 | 57 | 74 | None | Low or medium carbon steel |
| 2 | Over 3/4 to 1-1/2 | 33 | 36 | 60 | None | Low or medium carbon steel |
| 5 | 1/4 to 1 | 85 | 92 | 120 | 3 radial lines | Medium carbon steel, Q&T |
| 5 | Over 1 to 1-1/2 | 74 | 81 | 105 | 3 radial lines | Medium carbon steel, Q&T |
| 5.2 | 1/4 to 1 | 85 | 92 | 120 | Grade-specific mark | Low carbon martensitic (boron) steel, Q&T |
| 8 | 1/4 to 1-1/2 | 120 | 130 | 150 | 6 radial lines | Medium carbon alloy steel, Q&T |
| 8.2 | 1/4 to 1 | 120 | 130 | 150 | Grade-specific mark | Low carbon martensitic (boron) steel, Q&T |
Metric property classes (ISO 898-1 and ISO 3506)
Metric bolts do not use grades. They use a property class that encodes the strength directly in the number.
Figure 2
How to read a metric property class
| Class | Tensile, min MPa (ksi) | Yield or 0.2% proof, min MPa (ksi) | Typical material | Matching nut (ISO 898-2) |
|---|---|---|---|---|
| 4.6 | 400 (58) | 240 (35) | Low or medium carbon steel | Class 4 or 5 |
| 4.8 | 420 (61) | 340 (49) | Low or medium carbon steel | Class 5 |
| 5.8 | 520 (75) | 420 (61) | Low or medium carbon steel | Class 5 |
| 8.8 (to M16) | 800 (116) | 640 (93) | Medium carbon steel, Q&T | Class 8 |
| 8.8 (over M16) | 830 (120) | 660 (96) | Medium carbon steel, Q&T | Class 8 |
| 9.8 (to M16) | 900 (131) | 720 (104) | Medium carbon steel, Q&T | Class 9 |
| 10.9 | 1,040 (151) | 940 (136) | Alloy or boron steel, Q&T | Class 10 |
| 12.9 | 1,220 (177) | 1,100 (160) | Alloy steel, Q&T | Class 12 |
| Stainless (ISO 3506-1), A2 = 304-type, A4 = 316-type | ||||
| A2-50, A4-50 | 500 (73) | 210 (30) | Austenitic stainless, soft | Same group and class |
| A2-70, A4-70 | 700 (102) | 450 (65) | Austenitic stainless, cold worked | Same group and class |
| A2-80, A4-80 | 800 (116) | 600 (87) | Austenitic stainless, highly cold worked | Same group and class |
Metric nuts are classed by a single number that matches the first number of the bolt class: a class 10 nut for a class 10.9 bolt. Metric pressure bolting is usually ordered to ASTM A193M, A194M and A320M, or to European material standards. In those standards, 42CrMo4 is the chemistry closest to the 4140 steel used for B7.
Stainless and nickel alloy bolting
Stainless and nickel alloy bolting is ordered either to a bolting specification or to the bar specification it is machined from. The two routes give different testing and certification, so the drawing or purchase order should say which one applies.
| Specification | Covers | Common alloys | Notes |
|---|---|---|---|
| ASTM F593 / F594 | Stainless bolts, screws and studs / nuts, 1/4 to 1-1/2 in. | Group 1 (304 family), Group 2 (316 family), others | Condition CW1 (to 5/8 in.): 100 to 150 ksi tensile, 65 ksi yield. CW2 (3/4 to 1-1/2 in.): 85 to 140 ksi, 45 ksi yield. General use, not pressure bolting. |
| ASTM A193 / A320 B8 series | Stainless studs and bolts for pressure service | B8 (304), B8M (316), B8T (321), B8C (347) | State Class 1 or Class 2. Used where the piping code calls for A193 or A320. |
| ASTM F467 / F468 | Nonferrous nuts / bolts, screws and studs for general use | Nickel alloys, copper alloys, aluminum, titanium | Grade names follow the alloy, for example F468 Alloy 400 or 625. |
| ASTM B bar specifications | Bar the bolting is machined from | B164 (Monel 400), B865 (K-500), B446 (Inconel 625), B637 (Inconel 718), B425 (Incoloy 825), B574 (Hastelloy C-276), B473 (Alloy 20) | Strength depends on the condition: annealed, cold worked or age hardened. State it on the order. |
| ASTM A276 / A479 | Stainless and duplex bar | Duplex 2205, Super Duplex 2507, 254 SMO | Common bar specifications for duplex and super austenitic bolting. |
For corrosion and temperature screening across these alloys, use our Metallurgy Selector or the Fastener Materials Matrix.
Comparing grades across systems
Figure 3
Minimum strength of common bolting grades
Grades of similar strength are often treated as rough equivalents. The table below is a starting point for cross-referencing only. Each specification has its own testing, size range, marking and nut pairing, so a substitution should be approved by the engineer or purchaser.
| Strength level | ASTM | SAE | Metric | Approx. tensile, min |
|---|---|---|---|---|
| Low strength carbon steel | A307 Gr A | Grade 1, Grade 2 (over 3/4 in.) | 4.6, 4.8 | 58 to 61 ksi (400 to 420 MPa) |
| Medium strength, Q&T | A449, F3125 A325 | Grade 5 | 8.8 | 116 to 120 ksi (800 to 830 MPa) |
| High strength, Q&T alloy | A354 BD, F3125 A490 | Grade 8 | 10.9 | 150 ksi (1,040 MPa) |
| Very high strength | A574 socket head cap screws | – | 12.9 | About 170 to 180 ksi (1,220 MPa) |
| Pressure bolting | A193 B7, A320 L7 | – | A193M B7, A320M L7 (same grade, SI units) | 125 ksi (860 MPa) to 2-1/2 in. |
| Stainless, soft | A193 B8 / B8M Class 1 | – | A2-50 / A4-50 | 73 to 75 ksi (500 to 515 MPa) |
| Stainless, cold worked | F593 CW, A193 B8 / B8M Class 2 | – | A2-70 / A4-70, A2-80 / A4-80 | 100 to 125 ksi (700 to 860 MPa) |
Strength is only half the choice. Temperature range decides where each material can be used:
Figure 4
Typical service temperature ranges
Head and end markings
Most specifications require a grade mark and the manufacturer’s identification mark. Bolts and cap screws are marked on the head, studs on one end, and nuts on one face.
Figure 5
Common grade markings
A marking shows what the part claims to be. The mill test report, traced to the heat number, is the proof. Patriot Bolt also verifies alloy chemistry in house with XRF analysis.
Ordering checklist
- Specification, grade and class, for example ASTM A193 Grade B8M Class 2, or SAE J429 Grade 8, or ISO 898-1 class 10.9.
- Size, thread and length, for example 1-8UNC × 7-1/2 in., or M24 × 3 × 180 mm.
- Nut specification and grade, for example ASTM A194 Grade 2H heavy hex.
- Supplementary requirements, such as impact testing, NACE MR0175 / ISO 15156 hardness limits or 100% hardness testing.
- Coating or finish, such as PTFE, zinc-nickel or hot-dip galvanizing. See Fastener Coatings.
- Certification: mill test reports with heat numbers and a certificate of conformance.
Common questions
Is SAE Grade 8 the same as metric class 10.9?
They are close but not identical. Grade 8 has 150 ksi minimum tensile and 130 ksi yield. Class 10.9 has 1,040 MPa (about 151 ksi) tensile and 940 MPa (about 136 ksi) yield. The thread forms, sizes and markings differ, so one is not a drop-in replacement for the other.
Can A193 B7 replace SAE Grade 5 or A449?
B7 meets or beats Grade 5 strength in most sizes, and it is often supplied where a higher-strength stud is acceptable. It is a different specification with different testing and marking, so it should only be substituted when the drawing or the engineer allows it.
What is the difference between A193 and A320?
A193 covers bolting for high-temperature or high-pressure service. A320 covers bolting for low-temperature service and adds Charpy impact testing, for example L7 tested at −150 °F.
Why do strength values drop with diameter?
Quenching cannot harden the center of a large bar as fully as a small one. Most specifications therefore set lower minimums for larger diameters, for example B7 is 125 ksi tensile to 2-1/2 in. and 115 ksi over 2-1/2 to 4 in.
Do I need a class for stainless studs?
Yes. A193 B8 or B8M without a class is ambiguous. Class 1 (about 30 ksi yield) and Class 2 (up to 95 or 100 ksi yield in small sizes) are very different studs. Always state the class on the order.
Need bolting to a specific spec? Patriot Bolt machines stud bolts, bolts and nuts to ASTM and SAE specifications from B7 and B7M to stainless and nickel alloys, with mill test reports on every order. Send us the specification and grade from your drawing or bolting list. Request a quote or call (281) 581-0176.